EN 1.4404 Standard.pdf

May 06, 2025

Gadewch neges

EN 1.4404 Standard.pdf

info-280-280

Cyfansoddiad cemegol EN 1.4404 (x2crnimo 17-12-2)

Elfen C Si Mn P S N Cr Mo NI
% max 0.030 1.00 2.00 0.045 0.015¹ 0.10 16.50–18.50 2.00–2.50 10.00–13.00

Ar gyfer gwell machinability, caniateir cynnwys sylffwr rheoledig o {{0}}. 015–0.030%.

Priodweddau mecanyddol EN 1.4404 ar dymheredd yr ystafell (cyflwr anelio datrysiad)

Ffurflen Max. Trwch (mm) Cryfder Cynnyrch Rp 0. 2 (MPA) Cryfder Cynnyrch Rp1. 0 (MPA) Cryfder tynnol rm (mpa) Elongation A (%) Effaith Ynni ISO-V (J)
          Hydredol \/ traws Hydredol \/ traws
C Llai na neu'n hafal i 8 240 270 530–680 40 / - - / -
H Llai na neu'n hafal i 13.5 220 260 530–680 40 / - 100 / 60
P Llai na neu'n hafal i 75 220 260 520–670 45 / - 100 / 60
L Llai na neu'n hafal i 160 200 235 500–700 40 / - 100 / -
L Llai na neu'n hafal i 250² 200 235 500–700 - / 30 - / 60
TW\/S. Llai na neu'n hafal i 60 190 240 490–690 40 / 30 100 / 60⁷

Priodweddau ffisegol en 1.4404 dur gwrthstaen

Eiddo Gwerthfawrogom
Dwysedd ar 20 gradd (kg\/dm³) 8.0
Modwlws hydwythedd ar 20 gradd (kN\/mm²) 200
Dargludedd thermol ar 20 gradd (w\/m · k) 15
Capasiti thermol penodol ar 20 gradd (J\/kg · K) 500
Gwrthiant trydanol penodol ar 20 gradd (ω · mm²\/m) 0.75

EN 1.4404 Cyfernod llinellol dur gwrthstaen o ehangu thermol (10⁻⁶ K⁻¹)

Nhymheredd Gwerth (10⁻⁶ k⁻¹)
20 gradd i 100 gradd 16.0
200 gradd 16.5
300 gradd 17.0
400 gradd 17.5
500 gradd 18.0

EN 1.4404 Triniaeth Gwres Dur Di -staen

Tymheredd ffurfio poeth(gradd)) Dull oeri Triniaeth Gwres (Datrysiad wedi'i anelio)(gradd)) Dull oeri Microstrwythur
1150 i 850 Aeria ’ 1030 i 1110 Dŵr, aer Austenite gyda chynnwys ferrite isel

Anfon ymchwiliad