Cyfansoddiad Cemegol Dur Di-staen 304

Tabl 1 .Cyfansoddiad cemegol ar gyfer 304 o aloion dur di-staen

%

304

304L

304H

C

0.0 - 0.07

0.0 - 0.03

0.04 - 0.08

Mn

0.0 - 2.0

0.0 - 2.00

0.0 - 2.0

Si

0.0 - 1.00

0.0 - 1.00

0.0 - 1.0

P

0.0 - 0.05

0.0 - 0.05

0.0 - 0.04

S

0.0 - 0.03

0.0 - 0.02

0.0 - 0.02

Cr

17.50 - 19.50

17.50 - 19.50

17.00 - 19.00

Ni

8.00 - 10.50

8.00 - 10.50

8.00 - 11.00

Fe

Cydbwysedd

Cydbwysedd

Cydbwysedd

N

0.0-0.11

0.0-0.11

0.0 - 0.10

 

Priodweddau Dur Di-staen 304

Priodweddau Mecanyddol Dur Di-staen 304

Tabl 2a.Priodweddau mecanyddol ar gyfer 304 o aloion dur di-staen - dalen hyd at 8 mm o drwch

Gradd

304

304L

304H

Cryfder Tynnol (MPa)

540 - 750

520 - 700

-

Prawf Straen (MPa)

230 Munud

220 Munud

-

Elongation A50 mm

45 Munud %

45 Munud %

-


Tabl 2b.Priodweddau mecanyddol ar gyfer 304 o aloion dur gwrthstaen - plât o 8 - 75 mm o drwch

Gradd

304

304L

304H

Cryfder Tynnol (MPa)

520 - 720

500 - 700

-

Prawf Straen (MPa)

210 Munud

200 Munud

-

Elongation A5

45 Munud %

45 Munud %

-


Tabl 2c.Priodweddau mecanyddol ar gyfer 304 o aloion dur gwrthstaen - bar ac adran hyd at 160 mm o ddiamedr / trwch

Gradd

304

304L

304H

Cryfder Tynnol (MPa)

500 - 700

500 - 700

500 - 700

Prawf Straen (MPa)

190

175 Min

185 Min

Elongation A50 mm

45 Munud %

45 Munud %

40 Munud %

Caledwch Brinell

215 Uchafswm HB

215 Uchafswm HB

-